sus420j2不锈钢的硬度是多少 sus420j2不锈钢的硬度是多少?

420J2\u662f\u4ec0\u4e48\u6750\u6599\u4e0d\u9508\u94a2420J2\u7684\u786c\u5ea6\u662f\u591a\u5c11

420J2\u7684\u6027\u80fd\u548c\u7528\u9014\u548c420J2\u7c7b\u4f3c\uff0c\u4f46\u5f3a\u5ea6\u548c\u786c\u5ea6\u9ad8\u4e8e420J2\uff083cr13\uff09\uff0c\u4f46\u97e7\u6027\u548c\u8010\u8680\u6027\u7565\u4f4e\u4e9b\u3002\u710a\u63a5\u6027\u80fd\u5dee\u901a\u5e38\u4e0d\u4f5c\u710a\u63a5\u90e8\u4ef6\u3002

\u4e00\u3001420J2\u5bf9\u5e94\u724c\u53f7\uff1a1\u3001\u56fd\u6807GB-T\u6807\u51c6\uff1a\u6570\u5b57\u724c\u53f7\uff1aS42040\u3001\u65b0\u724c\u53f7\uff1a40Cr13\u3001\u65e7\u724c\u53f7\uff1a4Cr13,2\u3001\u7f8e\u6807\uff1aASTMA\u6807\u51c6\uff1a\u4e00\uff0cSAE\u6807\u51c6\uff1a\u4e00\uff0cUNS\u6807\u51c6\uff1a420J2\uff0c3\u3001\u65e5\u6807JIS\u6807\u51c6\uff1a420\uff0c4\u3001\u5fb7\u6807DIN\u6807\u51c6\uff1a1.4031,5\u3001\u6b27\u6807EN\u6807\u51c6\uff1aX39Cr13\u3002

\u4e8c\u3001420J2\u5316\u5b66\u6210\u5206\uff1a\u2474\u78b3C\uff1a0.36~0.45\uff0c\u2475\u7845Si\uff1a\u22641.00\uff0c\u2476\u9530Mn\uff1a\u22641.00\uff0c\u2477\u78f7P\uff1a\u22640.040\uff0c\u2478\u786bS\uff1a\u22640.030\uff0c\u2479\u94ecCr\uff1a12.50\uff5e14.50\uff0c\u247a\u954dNi\uff1a\u5145\u8bb8\u52a0\u22650.60\uff0c\u247b\u94bcMo\uff1a\u2014\uff0c\u247c\u6c2eN\uff1a\u2014\uff0c\u247d\u94dcCu\uff1a\u2014\uff0c\u247e\u5176\u5b83\u5143\u7d20\uff1a\u2014\u3002

\u4e09\u3001420J2\u7269\u7406\u6027\u80fd\uff1a\u2460\u5bc6\u5ea6\u5bc6\u5ea6(20\u2103)
/kg/dm3:7.75,\u2461\u7194\u70b9/\u2103:\u2014,\u2462\u6bd4\u70ed\u5bb9(0~100\u2103)/kg/(kg.k):0.46,\u2463\u70ed\u5bfc\u7387/w/(m.k)
100\u2103-:28.1,\u2478\u70ed\u5bfc\u7387/w/(m.k)
500\u2103-:28.9,\u2465\u7ebf\u80c0\u7cfb\u6570
/(10-6/k)
0~100\u2103:10.5,\u2466\u7ebf\u80c0\u7cfb\u6570/(10-6/k)
0~596\u2103:
12,\u2467\u7535\u963b\u7387\uff0820\u2103\uff09
/\uff08\u03a9.mm2/m):0.59,\u2468\u7eb5\u5411\u5f39\u6027\u6a21\u91cf
\uff0820\u2103\uff09/GPa:215\uff0c\u2469\u78c1\u6027:\u6709\u3002

\u56db\u3001420J2\u529b\u5b66\u6027\u80fd:\u2474\u4ea4\u8d27\u72b6\u6001\uff1a\u68d2\u6750\u56fa\u6eb6\u5904\u7406\uff0c\u677f\u6750\u56fa\u6eb6\u9178\u6d17\uff0c\u2475\u6297\u62c9\u5f3a\u5ea6\uff08RM/MPa\uff09\uff1a590\uff0c\u2476\u5ef6\u4f38\u5f3a\u5ea6\uff08Rp0.2/MPa\uff09\uff1a225\uff0c\u2477\u4f38\u957f\u7387A/%\uff1a15\uff0c\u2478\u65ad\u9762\u6536\u7f29\u7387\uff08Z/%\uff09\uff1a-\u3002

\u4e94\u3001420J2\u70ed\u5904\u7406\uff1a\u2460\u786c\u5ea6HBW\u2264\uff1a\u9000\u706b201\uff0c\u786c\u5ea6HRB\u2264\uff1a\u6dec\u706b\u56de\u706b50HRC\uff0c\u2461\u52a0\u70ed\u6e29\u5ea6\uff1a800~900\uff0c\u2462\u52a0\u70ed\u65b9\u5f0f\uff1a\u7a7a\u51b7\u6216\u7f13\u51b7\u3002

420J2\u5e94\u7528\u9886\u57df\uff1a\u4e3b\u8981\u5236\u4f5c\u5916\u79d1\u7528\u5177\uff0c\u8f74\u627f\uff0c\u9600\u95e8\uff0c\u5f39\u7c27\u7b49\u3002

420J2\u7684\u6027\u80fd\u548c\u7528\u9014\u548c420J2\u7c7b\u4f3c\uff0c\u4f46\u5f3a\u5ea6\u548c\u786c\u5ea6\u9ad8\u4e8e420J2\uff083cr13\uff09\uff0c\u4f46\u97e7\u6027\u548c\u8010\u8680\u6027\u7565\u4f4e\u4e9b\u3002\u710a\u63a5\u6027\u80fd\u5dee\u901a\u5e38\u4e0d\u4f5c\u710a\u63a5\u90e8\u4ef6\u3002

\u4e00\u3001420J2\u5bf9\u5e94\u724c\u53f7\uff1a1\u3001\u56fd\u6807GB-T\u6807\u51c6\uff1a\u6570\u5b57\u724c\u53f7\uff1aS42040\u3001\u65b0\u724c\u53f7\uff1a40Cr13\u3001\u65e7\u724c\u53f7\uff1a4Cr13,2\u3001\u7f8e\u6807\uff1aASTMA\u6807\u51c6\uff1a\u4e00\uff0cSAE\u6807\u51c6\uff1a\u4e00\uff0cUNS\u6807\u51c6\uff1a420J2\uff0c3\u3001\u65e5\u6807JIS\u6807\u51c6\uff1a420\uff0c4\u3001\u5fb7\u6807DIN\u6807\u51c6\uff1a1.4031,5\u3001\u6b27\u6807EN\u6807\u51c6\uff1aX39Cr13\u3002

\u4e8c\u3001420J2\u5316\u5b66\u6210\u5206\uff1a\u2474\u78b3C\uff1a0.36~0.45\uff0c\u2475\u7845Si\uff1a\u22641.00\uff0c\u2476\u9530Mn\uff1a\u22641.00\uff0c\u2477\u78f7P\uff1a\u22640.040\uff0c\u2478\u786bS\uff1a\u22640.030\uff0c\u2479\u94ecCr\uff1a12.50\uff5e14.50\uff0c\u247a\u954dNi\uff1a\u5145\u8bb8\u52a0\u22650.60\uff0c\u247b\u94bcMo\uff1a\u2014\uff0c\u247c\u6c2eN\uff1a\u2014\uff0c\u247d\u94dcCu\uff1a\u2014\uff0c\u247e\u5176\u5b83\u5143\u7d20\uff1a\u2014\u3002

\u4e09\u3001420J2\u7269\u7406\u6027\u80fd\uff1a\u2460\u5bc6\u5ea6\u5bc6\u5ea6(20\u2103)
/kg/dm3:7.75,\u2461\u7194\u70b9/\u2103:\u2014,\u2462\u6bd4\u70ed\u5bb9(0~100\u2103)/kg/(kg.k):0.46,\u2463\u70ed\u5bfc\u7387/w/(m.k)
100\u2103-:28.1,\u2478\u70ed\u5bfc\u7387/w/(m.k)
500\u2103-:28.9,\u2465\u7ebf\u80c0\u7cfb\u6570
/(10-6/k)
0~100\u2103:10.5,\u2466\u7ebf\u80c0\u7cfb\u6570/(10-6/k)
0~596\u2103:
12,\u2467\u7535\u963b\u7387\uff0820\u2103\uff09
/\uff08\u03a9.mm2/m):0.59,\u2468\u7eb5\u5411\u5f39\u6027\u6a21\u91cf
\uff0820\u2103\uff09/GPa:215\uff0c\u2469\u78c1\u6027:\u6709\u3002

\u56db\u3001420J2\u529b\u5b66\u6027\u80fd:\u2474\u4ea4\u8d27\u72b6\u6001\uff1a\u68d2\u6750\u56fa\u6eb6\u5904\u7406\uff0c\u677f\u6750\u56fa\u6eb6\u9178\u6d17\uff0c\u2475\u6297\u62c9\u5f3a\u5ea6\uff08RM/MPa\uff09\uff1a590\uff0c\u2476\u5ef6\u4f38\u5f3a\u5ea6\uff08Rp0.2/MPa\uff09\uff1a225\uff0c\u2477\u4f38\u957f\u7387A/%\uff1a15\uff0c\u2478\u65ad\u9762\u6536\u7f29\u7387\uff08Z/%\uff09\uff1a-\u3002

\u4e94\u3001420J2\u70ed\u5904\u7406\uff1a\u2460\u786c\u5ea6HBW\u2264\uff1a\u9000\u706b201\uff0c\u786c\u5ea6HRB\u2264\uff1a\u6dec\u706b\u56de\u706b50HRC\uff0c\u2461\u52a0\u70ed\u6e29\u5ea6\uff1a800~900\uff0c\u2462\u52a0\u70ed\u65b9\u5f0f\uff1a\u7a7a\u51b7\u6216\u7f13\u51b7\u3002

420J2\u5e94\u7528\u9886\u57df\uff1a\u4e3b\u8981\u5236\u4f5c\u5916\u79d1\u7528\u5177\uff0c\u8f74\u627f\uff0c\u9600\u95e8\uff0c\u5f39\u7c27\u7b49\u3002

sus420j2不锈钢,相当于我国的马氏体型不锈钢 3Cr13,出厂时一般为退火状态热处理硬度为小于等于布氏硬度|HB235。热处理淬火后,硬度可达洛氏硬度HRC48-55。



sus420j2不锈钢,相当于我国的马氏体型不锈钢 3Cr13,出厂时一般为退火状态热处理硬度为小于等于布氏硬度|HB235。热处理淬火后,硬度可达洛氏硬度HRC48-55。

标准:JIS G 4303:2005
属马氏体类型不锈钢,该钢机械加工性能好
调质处理后硬度在HRC30以下的3Cr13材料加工性较好,易达到较好的表面质量。
而硬度大于HRC30时加工出的零件,表面质量虽然较好,但刀具易磨损。
所以,在材料进厂后,先进行调质处理硬度达到HRC25~30,然后再进行切削加工。
比SUS420J2淬火后的硬度高,作刃具、喷嘴、阀座、阀门等。
SUS420J2密度为7.75g/cm3。

420J2的性能和用途和420J2类似,但强度和硬度高于420J2(3cr13),但韧性和耐蚀性略低些。焊接性能差通常不作焊接部件。

一、420J2对应牌号:1、国标GB-T标准:数字牌号:S42040、新牌号:40Cr13、旧牌号:4Cr13,2、美标:ASTMA标准:一,SAE标准:一,UNS标准:420J2,3、日标JIS标准:420,4、德标DIN标准:1.4031,5、欧标EN标准:X39Cr13。

二、420J2化学成分:⑴碳C:0.36~0.45,⑵硅Si:≤1.00,⑶锰Mn:≤1.00,⑷磷P:≤0.040,⑸硫S:≤0.030,⑹铬Cr:12.50~14.50,⑺镍Ni:充许加≥0.60,⑻钼Mo:—,⑼氮N:—,⑽铜Cu:—,⑾其它元素:—。

三、420J2物理性能:①密度密度(20℃)
/kg/dm3:7.75,②熔点/℃:—,③比热容(0~100℃)/kg/(kg.k):0.46,④热导率/w/(m.k)
100℃-:28.1,⑸热导率/w/(m.k)
500℃-:28.9,⑥线胀系数
/(10-6/k)
0~100℃:10.5,⑦线胀系数/(10-6/k)
0~596℃:
12,⑧电阻率(20℃)
/(Ω.mm2/m):0.59,⑨纵向弹性模量
(20℃)/GPa:215,⑩磁性:有。

四、420J2力学性能:⑴交货状态:棒材固溶处理,板材固溶酸洗,⑵抗拉强度(RM/MPa):590,⑶延伸强度(Rp0.2/MPa):225,⑷伸长率A/%:15,⑸断面收缩率(Z/%):-。

五、420J2热处理:①硬度HBW≤:退火201,硬度HRB≤:淬火回火50HRC,②加热温度:800~900,③加热方式:空冷或缓冷。

420J2应用领域:主要制作外科用具,轴承,阀门,弹簧等。

硬度HBW:退火235,淬火回火217
硬度HRB:99

  • 鑺辩敯娲嬬殑浠h〃浜у搧
    绛旓細鍦ㄥ畼缃戜笅杞戒簡HIGO-S鐨凱DF浠嬬粛鏂囦欢锛岄噷闈粙缁SUS420j2涓嶉攬閽㈢殑纭害鏄Hrc60銆傝屽叾瀹冪増鏈殑鑲ュ悗鎴栬呭叾瀹冨垁鍨嬩腑锛岄櫎浜嗛珮寮哄害閾濇潗澶栵紝鎵嬫焺鍙婅儗澶规墍閲囩敤鐨凷US402J2涓嶉攬閽紝鍏剁‖搴﹀彧鏈塇rc48鎴栬匟rc52锛屼笌SUS420j2涓嶉攬閽㈢殑鎬ц兘骞朵笉鐩稿悓銆傛嵁璇撮搧鏈ㄦ槸涓绉嶄粎鐢熼暱鍦ㄧ編鍥借タ鍗楅儴鍒板ⅷ瑗垮摜瑗垮寳閮ㄦ矙婕犱腑鐨勭亴鏈ㄥ皬涔旀湪銆傜敱浜庢矙婕...
  • SUS420J2鏄浠涔堝寲瀛︽垚鍒
    绛旓細420J2鐨勬ц兘鍜岀敤閫斿拰420J2绫讳技锛屼絾寮哄害鍜纭害楂樹簬420J2锛3cr13锛夛紝浣嗛煣鎬у拰鑰愯殌鎬х暐浣庝簺銆傜剨鎺ユц兘宸氬父涓嶄綔鐒婃帴閮ㄤ欢銆備竴銆420J2瀵瑰簲鐗屽彿锛1銆佸浗鏍嘒B-T鏍囧噯锛氭暟瀛楃墝鍙凤細S42040銆佹柊鐗屽彿锛40Cr13銆佹棫鐗屽彿锛4Cr13,2銆佺編鏍囷細ASTMA鏍囧噯锛氫竴锛孲AE鏍囧噯锛氫竴锛孶NS鏍囧噯锛420J2锛3銆佹棩鏍嘕IS鏍囧噯锛420锛4銆佸痉鏍...
  • sus303涓sus420鏈変粈涔堝尯鍒
    绛旓細SUS420F2鍥涗釜绛夌骇鏉愭枡锛屽睘浜庢棩鏍囬┈姘忎綋涓嶉攬閽锛岀粡鐑鐞(娣伀鍥炵伀)鍚,鍏锋湁浼樿壇鐨勮愯厫铓鎬ц兘鎶涘厜鎬ц兘杈冮珮鐨勫己搴﹀拰鑰愮(鎬,閫傚疁鍒堕犳壙鍙楅珮璐熻嵎,楂樿愮(鍙婂湪鑵愯殌浠嬭川浣滅敤涓嬬殑濉戞枡妯″叿銆係US420J1銆SUS420J2銆丼US420F銆丼US420F2鍖栧鎴愬垎濡備笅鍥撅細SUS420J1銆丼US420J2銆丼US420F銆丼US420F2鍔涘鎬ц兘鍙纭害鍊煎涓嬪浘锛...
  • sus420鏄粈涔鏉愭枡,鍐插帇鐑鐞嗗悗纭害鍙互杈惧埌HRC澶氬皯?
    绛旓細SUS420鏄挗鏉愶紝棰勭‖鏄30-34HRC銆係US420閽㈡潗楂橀煣鎬э紝楂樼‖搴︾┖鍐锋番纭珮閾伐鍏烽挗锛屾瘮SKD閽㈡潗鐨勭‖搴鍙婇煣鎬уソ锛岄珮闀滈潰銆侀珮鑰愯殌銆傜儹澶勭悊灏哄鍙樺寲灏忋係US420瀹滅嚎鍓插姞宸ワ紝鐢ㄤ簬鍐插帇锛屾媺娣卞拰鎼撶墮妯¢珮闀滈潰楂樼簿瀵嗘ā鍏枫傛憚鍍忔満銆佸寲濡嗗鍣ㄣ侀忔槑缃╃被銆侀忔槑鑳剁墖绛夈
  • SUS420J2椹皬浣涓嶉攬閽鐑鐞嗗悗纭害鍋忎綆
    绛旓細SUS420J2鏄3Cr13锛纭害浣庢槸鍥炵伀娓╁害楂樹簡銆傛垨鑰呮槸娣伀鍐峰嵈鏃跺喎鍗撮熷害浣庛傛垚鍒嗗亸鏋愬彲鑳介犳垚纭害涓嶅潎鍖銆
  • 涓嶉攬閽420b鍥烘憾涔嬪悗鐨勭‖搴︽槸澶氬皯
    绛旓細SUS420J2娣伀娓╁害鍦1000~1050鈩冿紝鍥炵伀娓╁害鍦200~500鈩冦SUS420J2鏄椹皬浣撳瀷涓嶉攬閽锛屽湪娣伀鍥炵伀鍚庝娇鐢ㄣ備笌1Cr13銆2Cr13閽㈢浉瀵癸紝鏈夋洿楂樼殑寮哄害銆纭害鍜屾番閫忔э紝浣嗗叾鑰愯殌鎬у拰 700鈩 浠ヤ笅鐨勭儹绋冲畾鎬ц緝1Cr13銆2Cr13閽綆銆傚喎鍔犲伐鎬ц兘鍜岀剨鎺ユц兘涓嶅ソ锛岀剨鍚庡簲绔嬪嵆鐑鐞嗭紝浠ラ槻寮瑁傘傚湪閫鐏姸鎬佷笅鍏锋湁杈冨ソ鐨...
  • HPM38鏉愭枡鏈夌鎬у悧?
    绛旓細浣犺鐨勮繖娆綡PM38鏉愭枡鏄涓嶅叿澶囩鎬х殑銆備笅闈㈠氨浼氬叿浣撹瀹冩槸鐢变粈涔堟潗璐ㄦ瀯鎴愮殑锛屾棩绔嬮噾灞濰PM38(SUS420J2鏀硅壇)鏄13CR绯诲惈MO涓嶉攬閽,缁忚繃鐗规畩婧惰В鍒堕犺屾垚鏈夊緢濂界殑鑰愯厫铓鎬.閫傚悎浜庤姹纭害楂樹笖瀵硅愯厫铓闀滈潰鎬ц姹傞珮鐨勫鑳舵ā鍏,鑰屼笖,HPM38鐑鐞嗗昂瀵稿彉鍖栨瀬灏,閫傚悎绮惧瘑鐑鐞.HPM38鏃ユ湰鏃ョ珛閲戝睘濉戣兌妯″叿閽紝瓒呯骇闀滈潰...
  • 2083 鏉愭枡鐨勭‖搴︽槸澶氬皯搴
    绛旓細GS-2083涓哄痉鍥紻IN鏍囧噯妯″叿閽紝濉戣兌妯″叿閽2083妯″叿閽㈡槸寰峰浗DIN鏍囧噯鐗屽彿1.2083锛岀編鍥紸ISI鏍囧噯鐗屽彿涓420锛屾棩鏈琂IS鏍囧噯鐗屽彿SUS420J2锛岀憺鍏镐竴鑳滅櫨鏍囧噯鐗屽彿涓篠TAVAX鎾掓柉鐗2083棰勫姞纭槻閰稿鑳舵ā鍏烽挗锛屽竷寰烽瞾鏂2083涓洪珮鍚玞r涓嶉攬閽,鍚玞r楂樿揪15%浠ヤ笂锛屾嫢鏈夐潪甯稿嚭鑹茬殑鑰愮(鎬.闃查吀浠ュ強鑹ソ鐨勬姏鍏夋ц兘锛岀粡娣伀鍚庢洿鍏疯愮(...
  • SUS420,SUS420F纾侀搧鍙互鍚歌捣鏉ョ畻涓嶉攬閽鍚?
    绛旓細RM/MPa锛夛細735锛屸懚寤朵几寮哄害锛圧p0.2/MPa锛夛細540锛屸懛浼搁暱鐜嘇/%锛12锛屸懜鏂潰鏀剁缉鐜囷紙Z/%锛夛細40銆備簲銆丼US420F鐑鐞嗭細鈶纭害HBW鈮わ細閫鐏235锛屾番鐏洖鐏217锛岀‖搴RB鈮わ細99锛屸憽鍔犵儹娓╁害锛800~900锛屸憿鍔犵儹鏂瑰紡锛氱┖鍐锋垨缂撳喎銆係US420F搴旂敤棰嗗煙锛氱敤浜庤嚜鍔ㄨ溅搴婂姞宸ョ殑闆朵欢鍜屾爣鍑嗕欢锛屽铻烘爴锛岃灪甯界瓑銆
  • 3Cr13瀵瑰簲鐗屽彿鏄粈涔?纭害澶氬皯?
    绛旓細3Cr13姣410锛1cr13锛夊拰420J1(2cr13)杩樿楂樼殑寮哄害銆纭害銆佹番閫忔э紝鍦ㄥ娓╋紙700搴︼級鐨勭█HNO3鍜屽急鏈夋満閰镐腑鏈夎愯殌鎬э紝鍜岀剨鎺ユт笉鍙410鍜410J1銆備竴銆3Cr13瀵瑰簲鐗屽彿锛1銆佸浗鏍嘒B-T鏍囧噯锛氭暟瀛楃墝鍙凤細S42030銆佹柊鐗屽彿锛30Cr13銆佹棫鐗屽彿锛3Cr13,2銆佺編鏍囷細ASTMA鏍囧噯锛歋42080锛孲AE鏍囧噯锛氫竴锛孶NS鏍囧噯锛420锛...
  • 扩展阅读:硬度对照表图片 ... 12种不锈钢型号大全 ... 420不锈钢成分表 ... 不锈钢的硬度型号排名 ... 420不锈钢对应牌号 ... 不锈钢型号硬度对照表 ... 420不锈钢硬度对照表 ... 304硬度一般是多少 ... 不锈钢sus301硬度是多少 ...

    本站交流只代表网友个人观点,与本站立场无关
    欢迎反馈与建议,请联系电邮
    2024© 车视网